Got an anycubic resin printer and I’m using their high speed resin (because it was bundled for free), and i tried to send a file using the high speed setting.

After the print it was seemed to be ok, then after i left in a bath of ethanol (IPA can’t be found in stores in my country) i got all those holes.

What’s the problem?

A slicer problem? The ethanol bath? The high speed resin that’s not good?

  • @plandeka
    link
    English
    8
    edit-2
    9 months ago

    They look like air bubbles to me, but it is weird they only come out after the bath. Could be they were already inside, but only covered by a thin wall of resin.

    I usually use Isopropanol for bath not Ethanol, so I am not sure how your resin reacts with that. The bath should also be rather short, like 1min or something.

    A few things to try:

    • If you are shaking your resin before print, then give it like 10 minutes after you pour it into the vat, so all bubbles come out and pop
    • lower the print speed
    • add wait times between the end of lowering the plate and light on
    • try to hollow out the model if possible, so there is less printing volume